Stainless steel resists corrosion thanks to a very thin passive layer that forms spontaneously on its surface. Welding, heat treatment, grinding or contact with carbon steel tools damages this layer. The result: discolouration around the weld seam, rust spots on the surface and unexpected corrosion. Pickling and passivation are two different chemical treatments used to restore this layer.
What is pickling?
Pickling removes the coloured oxide layer (heat tint) formed by welding and heat treatment, together with the thin underlying metal layer whose corrosion resistance has been weakened. It removes a very small amount of metal and can give the surface a uniform, matt appearance.
What is passivation?
Passivation removes free iron and foreign iron contamination from the surface, supporting the formation of a sound, uniform passive layer. It does not remove heat tint or oxide layers, removes no metal and does not change the appearance of the surface.
Comparison
| Pickling | Passivation | |
|---|---|---|
| Purpose | Remove heat tint, scale and the weakened surface layer | Remove free iron, strengthen the passive layer |
| Metal removal | Yes (small amount) | Negligible |
| Appearance | Matt, uniform | Unchanged |
| When? | After welding, heat treatment, hot forming | After machining, grinding, contact with carbon steel; as a complement after pickling |
Application methods
- Immersion: Small and medium-sized parts, series production; the most uniform result.
- Paste / gel: Weld seams, tanks and large structures; applied by brush to the seam area only.
- Spray: Fast application on large surfaces.
- Electrolytic weld cleaning: Fast, local cleaning of the weld seam with a dedicated device.
With every method, rinse thoroughly with water after treatment and leave no product residue.
Occupational safety
Pickling products are strong chemicals and can be seriously hazardous to the skin, eyes and respiratory tract. Wear suitable gloves, a face shield and protective clothing, ventilate the work area well and follow the first-aid and handling instructions in the safety data sheet (SDS) strictly.
Quality control
- Visual inspection: Heat tint and stains must be completely removed.
- Humidity test: No rust spots should form on a surface kept in humidity for a set period.
- Free iron tests: Checking whether foreign iron remains on the surface.
- Specifications: Standards such as ASTM A380 and ASTM A967 are common references for pickling and passivation.
Frequently asked questions
Is it enough to remove weld discolouration with abrasive paper?
Although sanding visibly removes the colour, it cannot fully remove the weakened layer underneath and can contaminate the surface with iron. Pickling, or at least passivation, should follow.
Is passivation needed after pickling?
After pickling the surface already begins to passivate; however, an additional passivation step may be required in critical applications and by some specifications.
Support for pickling and passivation
Molkim offers pickling and passivation products in immersion, paste, gel and spray form. If you share the material grade, welding method and application conditions, we can determine the right product together.