PVD (physical vapour deposition) coatings are only a few microns thick and reflect the condition of the substrate surface exactly. Ion cleaning (etching) inside the vacuum chamber is a final activation step; it cannot remove macroscopic contamination such as oil, oxide or particles. For this reason, delamination, flaking, colour variation and spot defects are usually caused not by the coating process but by insufficient cleaning before coating.
What is on the surface before PVD?
- Organic contamination: Machining oils, cutting fluids, rust-preventive films, fingerprints, polishing and grinding compounds.
- Inorganic contamination: Oxide layers, heat tint, limescale and water spots, hardening salts.
- Particles: Grinding dust, blasting residue, chips, fibres and dust.
- Hidden contamination: Liquids trapped in blind holes, threads and pores. These cause outgassing in vacuum and coating defects.
Typical PVD pre-cleaning line
- Pre-degreasing: An alkaline ultrasonic bath where the heavy oil load is removed. Solvent or hybrid pre-cleaning can also be used for heavily soiled parts.
- Main cleaning: Alkaline ultrasonic cleaning. This is the step where polishing compound and grinding residues are actually removed.
- Rinsing: Intermediate rinse with tap water.
- Activation / oxide removal (if required): Removal of the thin oxide film with a suitable activation step. Chosen according to the material; on carbide tools, cobalt leaching must be avoided.
- Cascade rinsing with DI water: Two or three stages of deionised water to remove ionic residues. The conductivity of the final rinse should be monitored.
- Drying: Hot air or vacuum drying. For parts with blind holes, vacuum drying prevents water residue and staining.
- Contamination-free handling: Gloves, clean fixtures and covered transport. Cleaned parts should not be touched with bare hands and should go to coating without waiting.
Points to watch by substrate
| Substrate | Risk | Recommendation |
|---|---|---|
| Cemented carbide (WC-Co) | Dissolution of the cobalt binder (cobalt leaching), surface darkening | Cobalt-friendly cleaner; avoid long acidic contact |
| Tool steel, HSS | Flash rust | Fast drying after rinsing; temporary protection if needed |
| Stainless steel | Thin passive oxide film, water spots | Alkaline cleaning and DI water rinse, mild acidic activation if needed |
| Aluminium, titanium | Etching in alkaline media, discolouration | Low-alkaline or neutral cleaner suitable for these metals |
| Brass, chrome-plated decorative parts | Dulling, staining | Neutral or mild alkaline, short time, low temperature |
How is cleaning quality measured?
- Water break test: On a clean surface, water forms a continuous film; the film breaks on oily areas.
- Test inks / dyne pens: Quickly indicate surface energy.
- Tape test and white cloth test: For a simple check of particle and film residue.
- Post-coating adhesion tests: Rockwell indentation (VDI 3198) and scratch tests indirectly confirm the effectiveness of pre-cleaning.
- Final rinse conductivity: The higher the conductivity of the DI water, the greater the risk of ionic residue on the surface.
Common mistakes
- Using the cleaning bath for a long time without monitoring its oil load.
- Using tap water for the final rinse; salts left after drying cause stains and spot defects in the coating.
- Leaving parts exposed for a long time after cleaning.
- Insufficient rinsing and drying of blind holes and threads.
- Not fully neutralising and activating decoated parts before recoating.
Frequently asked questions
Why is chemical pre-cleaning needed when there is ion cleaning in the vacuum?
Ion cleaning only removes the final nanometre-level contamination and oxide. It cannot remove visible oil, compound or particle residue; these contaminants cause outgassing and adhesion failure in vacuum.
Why does the surface of carbide tools darken after cleaning?
At an unsuitable pH and temperature, the cobalt binder can dissolve from the surface. This weakens coating adhesion. Carbide-compatible cleaners that do not cause cobalt leaching should be used.
What water should be used for the final rinse before PVD?
Deionised (DI) or reverse osmosis (RO) water. Keeping the conductivity of the final rinse water low prevents drying stains and ionic residue.
Support for your PVD pre-cleaning line
Molkim offers chemical solutions for degreasing, main cleaning, activation and decoating steps before PVD coating. If you share your coating type, substrate material and information about your current line, we can evaluate the process steps and suitable chemicals together.
Related products: Ultrasonic and Immersion Bath Chemicals · Degreasing Chemicals · Paint and Coating Removal Chemicals · Contact